Rubidium Iodide (RbI)

♦ Rubidium Iodide (RbI) Data Sheet     ♦ Rubidium Iodide (RbI) MSDS

Rubidium Iodide has only specialist applications.

Transmission Range :0.3 to 50 μm
Refractive Index :1.609 at 10 μm (1)
Reflection Loss :10.4% at 10 μm (2 surfaces)
Absorption Coefficient :n/a
Reststrahlen Peak :n/a
dn/dT :-56 x 10-6/°C
dn/dμ = 0 :n/a
Density :3.55 g/cc
Melting Point :642°C
Thermal Conductivity :9.9 W m-1 K-1
Thermal Expansion :39 x 10-6 /°C at 283K
Hardness :n/a
Specific Heat Capacity :242 J Kg-1 K-1 at 283K
Dielectric Constant :n/a
Youngs Modulus (E) :n/a
Shear Modulus (G) :n/a
Bulk Modulus (K) :11 GPa
Elastic Coefficients :C11=27.6; C12=3.7; C44=2.79
Apparent Elastic Limit :n/a
Poisson Ratio :n/a
Solubility :152g/100g water
Molecular Weight :212.37
Class/Structure :Cubic FCC, NaCl, Fm3m, (100) cleavage

To download this data or our MSDS safety data sheet as a pdf, please click on the links at the top of the page.  To expand the transmission graphs, please click on the image.
µm   Noµm   Noµm   No
0.25   2.0590.35   1.7360.50   1.663
0.80   1.6311.00   1.6242.00   1.615
5.00   1.61210.0   1.60920.0   1.596
30.0   1.57340.0   1.53745.0   1.514
50.0   1.48655.0   1.45260.0   1.411

Rubidium Iodide is produced by the sealed-ampoule Stockbarger technique. RbI is the most deliquescent of the rubidium salts.
REFERENCES:
(1) Handbook Optical Constants, ed Palik, V3, ISBN 0-12-544423-0