Products › Materials › Zinc Sulphide FLIR (Zinc Sulfide) (ZnS)
|
|
|
Zinc Sulphide FLIR (Zinc Sulfide) (ZnS) |
| ZnS FLIR is used for IR windows and lenses in the thermal band (8 to 14 μm) as a tough front optic in thermal imaging systems, particularly those subjected to harsh environments. |
|
|
Product Data |
| Transmission Range : |
1.0 to 13 μm |
| Refractive Index : |
2.192 at 10.6 μm |
| Reflection Loss : |
24.6% at 10.6 μm (2 surfaces) |
| Absorption Coefficient : |
0.02 cm-1 at 3.8 μm |
| Reststrahlen Peak : |
30.5 μm |
| dn/dT : |
+43 x 10-6/°C at 3.39 μm |
| dn/dμ = 0 : |
n/a |
| Density : |
4.08 g/cc |
| Melting Point : |
1827°C (See notes below) |
| Thermal Conductivity : |
16.7 W m-1 K-1 at 296K |
| Thermal Expansion : |
6.6 x 10-6 /°C at 273K |
| Hardness : |
Knoop 160 with 50g indenter |
| Specific Heat Capacity : |
469 J Kg-1 K-1 |
| Dielectric Constant : |
n/a |
| Youngs Modulus (E) : |
74.5 GPa |
| Shear Modulus (G) : |
n/a |
| Bulk Modulus (K) : |
n/a |
| Elastic Coefficients : |
Noy Available |
| Apparent Elastic Limit : |
103.4 MPa (15,000 psi) |
| Poisson Ratio : |
0.29 |
| Solubility : |
65 x 10-6 g/100g water |
| Molecular Weight : |
97.43 |
| Class/Structure : |
Polycrystalline cubic, ZnS, F43m |
To download this data or our MSDS safety data sheet as a pdf, please click on the links at the top of the page. To expand the transmission graphs, please click on the image.
|
|
|
|
Refractive Index |
| µm |
No |
µm |
No |
µm |
No |
| 0.42 |
2.516 |
0.46 |
2.458 |
0.50 |
2.419 |
| 0.54 |
2.391 |
0.58 |
2.371 |
0.62 |
2.355 |
| 0.66 |
2.342 |
0.70 |
2.332 |
0.74 |
2.323 |
| 0.78 |
2.316 |
0.82 |
2.31 |
0.86 |
2.305 |
| 0.90 |
2.301 |
0.94 |
2.297 |
0.98 |
2.294 |
| 1.00 |
2.292 |
1.40 |
2.275 |
1.80 |
2.267 |
| 2.20 |
2.263 |
2.60 |
2.26 |
3.00 |
2.257 |
| 3.40 |
2.255 |
3.80 |
2.253 |
4.20 |
2.251 |
| 4.60 |
2.248 |
5.00 |
2.246 |
5.40 |
2.244 |
| 5.80 |
2.241 |
6.20 |
2.238 |
6.60 |
2.235 |
| 7.00 |
2.232 |
7.40 |
2.228 |
7.80 |
2.225 |
| 8.20 |
2.221 |
8.60 |
2.217 |
9.00 |
2.212 |
| 9.40 |
2.208 |
9.80 |
2.203 |
10.2 |
2.198 |
| 10.6 |
2.192 |
11.0 |
2.186 |
11.4 |
2.18 |
| 11.8 |
2.173 |
12.2 |
2.167 |
12.6 |
2.159 |
| 13.0 |
2.152 |
13.4 |
2.143 |
13.8 |
2.135 |
| 14.2 |
2.126 |
14.6 |
2.116 |
15.0 |
2.106 |
| 15.4 |
2.095 |
15.8 |
2.084 |
16.2 |
2.072 |
| 16.6 |
2.059 |
17.0 |
2.045 |
17.4 |
2.03 |
| 17.8 |
2.015 |
18.2 |
1.998 |
|
|
Product Notes |
Zinc Sulphide is produced by synthesis from Zinc vapour and H2S gas, forming as sheets on Graphite susceptors. Zinc Sulphide is microcrystalline in structure, the grain size being controlled to produce maximum strength. Forward Looking Infra-Red (FLIR) grade, which is pale yellow and translucent in the visible, is used as deposited without further treatment. It is stronger than multispectral grade. Single crystal ZnS is available, but is not common.
ZnS oxidises significantly at 300°C, exhibits plastic deformation at about 500°C and dissociates about 700°C. For safety, Zinc Sulphide windows should not be used above 250°C in normal atmosphere.
|
|
|
Data provided is extracted from our technical handbook of materials. While every attempt has been made to verify the source of the information, Crystran Ltd accept no responsibility for accuracy of data |
|
Back to Materials
|
|
|
Membership Crystran Ltd is proud to be ISO 9001 certified through LRQA and ISO
14001 certified through SGS. |
| |
|