Strontium Fluoride has only specialist applications. Optically, Strontium Fluoride has properties intermediate to Calcium and Barium Fluoride.

Product Data

Transmission Range : 0.15 to 11 μm
Refractive Index : 1.439 at 0.55 μm (1)
Reflection Loss : 6.3% at 0.55 μm (2 surfaces)
Absorption Coefficient : <1 x 10-3 cm-1 at 5 μm
Reststrahlen Peak : 46 μm
dn/dT : -12 x 10-6 /°C
dn/dμ = 0 : n/a
Density : 4.24 g/cc
Melting Point : 1450°C
Thermal Conductivity : 1.42 W m-1 K-1 at 298K
Thermal Expansion : 18.4 x 10-6 /°C at 293K
Hardness : Knoop 154 (100) & 140 (110)
Specific Heat Capacity : 543 J Kg-1 K-1
Dielectric Constant : 7.69 at 2 MHz
Youngs Modulus (E) : 89.91 GPa
Shear Modulus (G) : 34.6 GPa
Bulk Modulus (K) : 24.65 GPa
Elastic Coefficients : C11=124; C12=45; C44=31.7
Apparent Elastic Limit : 36.5 MPa (5300 psi)
Poisson Ratio : 0.25
Solubility : 0.012g/100g water at 27°C
Molecular Weight : 125.62
Class/Structure : Cubic FCC, CaF2, Fm3m, (111) cleavage

To download this data or our MSDS safety data sheet as a pdf, please click on the links at the top of the page.  To expand the transmission graphs, please click on the image.

Click to access current Strontium Fluoride Stock Windows

Images

Strontium Fluoride IR Transmission Strontium Fluoride VUV Transmission

Refractive Index

µm    No µm    No µm    No
0.15    1.594 0.20    1.504 0.31    1.45725
0.41    1.44556 0.51    1.44029 0.61    1.43740
0.71    1.43560 0.81    1.43435 0.91    1.43343
1.01    1.43269 1.51    1.43003 2.01    1.42761
3.01    1.42159 4.01    1.41337 5.01    1.40269
6.01    1.38934 7.01    1.37308 8.01    1.35362
9.1    1.3283 10.1    1.3800 11.1    1.2686
12.35    1.3002

Product Notes

Strontium fluoride is produced by the vacuum Stockbarger growth technique.

REFERENCES:
(1) Handbook of Optical Constants, ed Palik, V3, ISBN 0-12-544423-0
Data provided is extracted from our technical handbook of materials. While every attempt has been made to verify the source of the information, Crystran Ltd accept no responsibility for accuracy of data
Back to Materials
Popular Downloads
Calcium Fluoride
Barium Fluoride
Germanium
Lithium Fluoride
Magnesium Fluoride
Quartz
Sapphire
Silicon
Zinc Selenide
Zinc Sulphide Cleartran

Membership


Crystran Ltd is proud to be ISO 9001 certified through LRQA and ISO 14001 certified through SGS.
UKAS