Products › Materials › Rubidium Bromide (RbBr)
|
|
|
Rubidium Bromide (RbBr) |
| Rubidium Bromide has only specialist applications. |
|
|
Product Data |
| Transmission Range : |
0.22 to 40 μm |
| Refractive Index : |
1.525 at 10 μm (1) |
| Reflection Loss : |
8.2% at 10 μm (2 surfaces) |
| Absorption Coefficient : |
1.6 x 10-3 cm-1 at 10.6 μm |
| Reststrahlen Peak : |
n/a |
| dn/dT : |
-45 x 10-6 /°C |
| dn/dμ = 0 : |
n/a |
| Density : |
3.35 g/cc |
| Melting Point : |
682°C |
| Thermal Conductivity : |
12.2 W m-1 K-1 at 378K |
| Thermal Expansion : |
36.98 x 10-6 /°C at 273K |
| Hardness : |
n/a |
| Specific Heat Capacity : |
311 J Kg-1 K-1 |
| Dielectric Constant : |
55 |
| Youngs Modulus (E) : |
n/a |
| Shear Modulus (G) : |
n/a |
| Bulk Modulus (K) : |
13.7 GPa |
| Elastic Coefficients : |
C11=31.5; C12=4.8; C44=3.82 |
| Apparent Elastic Limit : |
n/a |
| Poisson Ratio : |
n/a |
| Solubility : |
98g/100g water |
| Molecular Weight : |
165.38 |
| Class/Structure : |
Cubic FCC, NaCl, Fm3m, (100) cleavage |
To download this data or our MSDS safety data sheet as a pdf, please click on the links at the top of the page. To expand the transmission graphs, please click on the image.
|
|
|
|
Refractive Index |
| µm |
No |
µm |
No |
µm |
No |
| 0.240 |
1.754 |
0.350 |
1.603 |
0.400 |
1.583 |
| 0.500 |
1.563 |
0.600 |
1.552 |
0.70 |
1.546 |
| 0.80 |
1.543 |
0.90 |
1.540 |
1.00 |
1.538 |
| 2.00 |
1.533 |
5.00 |
1.530 |
10.0 |
1.525 |
| 15.0 |
1.517 |
20.0 |
1.505 |
25.0 |
1.489 |
| 30.0 |
1.469 |
35.0 |
1.444 |
40.0 |
1.412 |
|
|
Product Notes |
Rubidium Bromide is produced by the sealed-ampoule Stockbarger technique.
REFERENCES:
(1) Handbook Optical Constants, ed Palik, V3, ISBN 0-12-544423-0
|
|
|
Data provided is extracted from our technical handbook of materials. While every attempt has been made to verify the source of the information, Crystran Ltd accept no responsibility for accuracy of data |
|
Back to Materials
|
|
|
Membership Crystran Ltd is proud to be ISO 9001 certified through LRQA and ISO
14001 certified through SGS. |
| |
|