Rubidium Chloride (RbCl)
♦ Rubidium Chloride (RbCl) Data Sheet ♦ Rubidium Chloride (RbCl) MSDS
Rubidium Chloride has only specialist applications.
| Transmission Range : | 0.2 to 25 μm |
| Refractive Index : | 1.46 at 10.6 μm |
| Reflection Loss : | 6.8% at 10.6 μm (2 surfaces) |
| Absorption Coefficient : | 1 x 10-3 cm-1 at 10.6 μm |
| Reststrahlen Peak : | n/a |
| dn/dT : | -39 x 10-6/°C |
| dn/dμ = 0 : | n/a |
| Density : | 2.8 g/cc |
| Melting Point : | 715°C |
| Thermal Conductivity : | 7.6 W m-1 K-1 |
| Thermal Expansion : | 36 x 10-6 /°C at 300K |
| Hardness : | n/a |
| Specific Heat Capacity : | 418 J Kg-1 K-1 at 283K |
| Dielectric Constant : | 55 |
| Youngs Modulus (E) : | n/a |
| Shear Modulus (G) : | n/a |
| Bulk Modulus (K) : | 16.3 GPa |
| Elastic Coefficients : | C11=36.4; C12=6.3; C44=4.7 |
| Apparent Elastic Limit : | n/a |
| Poisson Ratio : | n/a |
| Solubility : | 77g/100g water |
| Molecular Weight : | 120.92 |
| Class/Structure : | Cubic FCC, NaCl, Fm3m, (100) cleavage |
To download this data or our MSDS safety data sheet as a pdf, please click on the links at the top of the page. To expand the transmission graphs, please click on the image.
| µm | No | µm | No | µm | No |
| 0.248 | 1.60 | 0.351 | 1.53 | 0.488 | 1.50 |
| 0.590 | 1.49 | 0.633 | 1.49 | 1.060 | 1.48 |
| 1.550 | 1.48 | 2.800 | 1.48 | 10.60 | 1.46 |
Rubidium Chloride is produced by the sealed-ampoule Stockbarger technique.