Products › Materials › Gallium Lanthanum Sulphide (GLS)
|
|
|
Gallium Lanthanum Sulphide (GLS) |
Gallium Lanthanum Sulphide is a radically new chalcogenide glass and a much awaited alternative to toxic Arsenic-based glasses, with an optical transparency from the visible to infrared wavelengths, and thermal stability up to 550oC. In addition, GLS can be melted in a large scale without the need for sealed ampoule processing making GLS production and processing safer and more economical. Equally important, impurity levels, in particular, OH- and SH- absorption bands at around 3 and 4 ìm have been substantially reduced thus increasing performance.
GLS has found use in a wide range of optoelectronic applications and is available as polished optical components, thin and thick films and in optical fibre form. See ChG Southampton Ltd for more information. |
|
|
Product Data |
| Transmission Range : |
0.5 to 10 μm |
| Refractive Index : |
2.398 at 1.014 μm |
| Reflection Loss : |
29% at 1.014 μm |
| Absorption Coefficient : |
<0.005 cm-1 |
| Reststrahlen Peak : |
n/a |
| dn/dT : |
+75 x 10-6 /°C |
| dn/dμ = 0 : |
4 μm |
| Density : |
4.04 g/cc |
| Melting Point : |
830°C |
| Thermal Conductivity : |
0.43 W cm-1 K-1 at 273K |
| Thermal Expansion : |
10 x 10-6 /°C at 273K |
| Hardness : |
Knoop 206 with 200g indenter |
| Specific Heat Capacity : |
0.54 J g-1 K-1 |
| Dielectric Constant : |
8.1 at 1KHz |
| Youngs Modulus (E) : |
59 GPa |
| Shear Modulus (G) : |
23 GPa |
| Bulk Modulus (K) : |
24.5 GPA |
| Elastic Coefficients : |
n/a |
| Apparent Elastic Limit : |
n/a |
| Poisson Ratio : |
0.24 |
| Solubility : |
Negligible in water |
| Molecular Weight : |
276.9 |
| Class/Structure : |
Amorphous glass |
To download this data or our MSDS safety data sheet as a pdf, please click on the links at the top of the page. To expand the transmission graphs, please click on the image.
|
|
|
|
Refractive Index |
| µm |
No |
µm |
No |
µm |
No |
| 0.5461 |
2.522 |
0.5790 |
2.500 |
0.6439 |
2.467 |
| 0.6678 |
2.458 |
0.7065 |
2.466 |
1.0140 |
2.398 |
| 1.3673 |
2.379 |
1.7101 |
2.371 |
|
|
Product Notes |
Gallium Lanthanum Sulphide (GLS) glass is produced by proprietary processes under conditions of the highest purity. Particular effort is made in removing transition metal impurities to a level of better than 1 ppm total metallic impurities with SH- and OH- less than 1 ppm. GLS is routinely processed from ingots of 500 grams. Other glass compositions are available including rare earth doped (Ce, Pr, Nd, Tb, Dy, Ho, Er, Tm, Yb), halide (F, Cl), and Ag doped samples.
Damage Threshold >200MW/cm2 at 1550nm
Acousto-optic Figure of Merit: M2 = 6 x 10-15
Verdet Constant = 0.205 min/Oe/cm
REFERENCES
Petrovich, Hewak et al Journal of Non-Crystalline Solids 326&327 (2003) 93–97
|
|
|
Data provided is extracted from our technical handbook of materials. While every attempt has been made to verify the source of the information, Crystran Ltd accept no responsibility for accuracy of data |
|
Back to Materials
|
|
|
Membership Crystran Ltd is proud to be ISO 9001 certified through LRQA and ISO