Gallium Arsenide (GaAs) Data Sheet
Gallium Arsenide (GaAs) MSDS

Gallium Arsenide (GaAs)

Gallium Arsenide has specialist applications in far IR optics and lens systems.

Product Data

Transmission Range : 1 to 16 μm (1)
Refractive Index : 3.2727 @ 10.33 μm (1)
Reflection Loss : 44% @ 10.33 μm
Absorption Coefficient : 0.01 cm-1
Reststrahlen Peak : n/a
dn/dT : 147 x 10-6/°C @ 10  μm (4)
dn/dμ = 0 : 6.3 μm
Density : 5.315 g/cc
Melting Point : 1511°C
Thermal Conductivity : 48 W m-1 K-1 @ 273K (2)
Thermal Expansion : 5.7 x 10-6 /°C at 300K (3)
Hardness : Knoop 750
Specific Heat Capacity : 360 J Kg-1 K-1
Dielectric Constant : 12.91 at low frequencies
Youngs Modulus (E) : 84.8 GPa
Shear Modulus (G) : n/a
Bulk Modulus (K) : 75.5 GPa
Elastic Coefficients : n/a
Apparent Elastic Limit : 71.9 MPa
Poisson Ratio : 0.31
Solubility : Insoluble in water
Molecular Weight : 144.64
Class/Structure : Cubic ZnS, F43m, (100) cleavage

To download this data or our MSDS safety data sheet as a pdf, please click on the links at the top of the page.  To expand the transmission graphs, please click on the image.

Images

Gallium Arsenide IR Transmission Gallium Arsenide NIR Transmission

Refractive Index

µm    No µm    No µm    No
1.033    3.492 1.550    3.3737 2.066    3.338
2.480    3.324 3.100    3.3125 4.133    3.3027
4.959    3.2978 6.199    3.2921 7.293    3.2874
8.266    3.2831 9.537    3.2769 10.33    3.2727
11.27    3.2671 12.40    3.2597 13.78    3.2493
15.50    3.2336 17.71    3.2081 19.07    3.1866

Product Notes

Gallium Arsenide is produced by Czochralski or horizontal Bridgeman crystal growth techniques. As it is arsenic bearing, precautions in handling and working should be observed.

REFERENCES:
(1) Handbook Optical Constants, ed Palik, V1, ISBN 0-12-544420-6
(2) Deutch, J.Electron. Mater. V4 p679
(3) Sze, Physics of Semiconductor Devices, Wiley 1981
(4) M.Cadona. Proc. Int Conf. Semicond. Phys. 1960 p.388
Data provided is extracted from our technical handbook of materials. While every attempt has been made to verify the source of the information, Crystran Ltd accept no responsibility for accuracy of data
Back to Materials
Popular Downloads
Calcium Fluoride
Barium Fluoride
Germanium
Lithium Fluoride
Magnesium Fluoride
Quartz
Sapphire
Silicon
Zinc Selenide
Zinc Sulphide Cleartran

Membership


Crystran Ltd is proud to be ISO 9001 certified through LRQA and ISO 14001 certified through SGS.
UKAS