Products › Materials › Caesium Iodide (Cesium Iodide) (CsI)
|
|
|
Caesium Iodide (Cesium Iodide) (CsI) |
| Caesium Iodide (Cesium Iodide) is the material with the deepest known IR transmission, and is sometimes used for components in the widest range spectrophotometers. An extremely soft material, Caesium Iodide is extremely difficult to polish, and so performance is compromised for range. Doped with Thallium, CsI(Tl) is a useful scintillator which emits at a wavelength that is a good match for Silicon photodiodes. Arrays of Caesium Iodide are used in security imaging systems. |
|
|
Product Data |
| Transmission Range : |
0.25 to 55 μm (1) |
| Refractive Index : |
1.73916 at 10 μm (1)(2) |
| Reflection Loss : |
13.6% at 10 μm |
| Absorption Coefficient : |
n/a |
| Reststrahlen Peak : |
145.8 μm |
| dn/dT : |
-99.3 x 10-6 /°C (2) |
| dn/dμ = 0 : |
6 μm |
| Density : |
4.51 g/cc |
| Melting Point : |
621 °C |
| Thermal Conductivity : |
1.1 W m-1 K-1 at 298 K (3) |
| Thermal Expansion : |
48.3 x 10-6 /°C at 293 K (3) |
| Hardness : |
Knoop 20 with 200g indenter |
| Specific Heat Capacity : |
201 J Kg-1 K-1 (4) |
| Dielectric Constant : |
5.65 at 1 MHz |
| Youngs Modulus (E) : |
5.3 GPa |
| Shear Modulus (G) : |
6.24 GPa |
| Bulk Modulus (K) : |
12.67 GPa |
| Elastic Coefficients : |
C11=24.6 C126.7 C44=6.24 |
| Apparent Elastic Limit : |
5.6 MPa (810psi) |
| Poisson Ratio : |
0.214 |
| Solubility : |
44 g/100 g water at 0 °C |
| Molecular Weight : |
259.83 |
| Class/Structure : |
Cubic CsCl, Pm3m, no cleavage, deforms |
To download this data or our MSDS safety data sheet as a pdf, please click on the links at the top of the page. To expand the transmission graphs, please click on the image.
|
|
|
|
Refractive Index |
| µm |
No |
µm |
No |
µm |
No |
| 0.5 |
1.8064 |
1.0 |
1.7572 |
2.0 |
1.7466 |
| 3.0 |
1.7440 |
4.0 |
1.7431 |
5.0 |
1.7424 |
| 6.0 |
1.7418 |
7.0 |
1.7412 |
8.0 |
1.7406 |
| 9.0 |
1.7399 |
10.0 |
1.7392 |
11.0 |
1.7384 |
| 12.0 |
1.7375 |
13.0 |
1.7365 |
14.0 |
1.7355 |
| 15.0 |
1.7344 |
16.0 |
1.7332 |
17.0 |
1.7319 |
| 18.0 |
1.7306 |
19.0 |
1.7291 |
20.0 |
1.7276 |
| 21.0 |
1.7260 |
22.0 |
1.7244 |
23.0 |
1.7226 |
| 24.0 |
1.7207 |
25.0 |
1.7188 |
26.0 |
1.7168 |
| 27.0 |
1.7147 |
28.0 |
1.7125 |
29.0 |
1.7101 |
| 30.0 |
1.7077 |
31.0 |
1.7052 |
32.0 |
1.7027 |
| 33.0 |
1.7000 |
34.0 |
1.6972 |
35.0 |
1.6943 |
| 36.0 |
1.6913 |
37.0 |
1.6882 |
38.0 |
1.6849 |
| 39.0 |
1.6816 |
40.0 |
1.6781 |
41.0 |
1.6746 |
| 42.0 |
1.6709 |
43.0 |
1.6671 |
44.0 |
1.6631 |
| 45.0 |
1.6591 |
46.0 |
1.6549 |
47.0 |
1.6505 |
| 48.0 |
1.6460 |
49.0 |
1.6414 |
50.0 |
1.6366 |
|
|
Product Notes |
Caesium Iodide is grown by sealed ampoule Stockbarger techniques with ingots of approximately 70mm diameter. CsI is very soft and pliable.
REFERENCES:
(1) Handbook Optical Constants, ed Palik, V2, ISBN 0-12-544422-2
(2) Rodney, J.Opt.Soc.Am. V45, p987, 1955
(3) Combes et al, J.Opt.Soc.Am. V41, p215, 1951
(4) Kelly, Bureau of Mines Bulletin, No371, p51, 1934
|
|
|
Data provided is extracted from our technical handbook of materials. While every attempt has been made to verify the source of the information, Crystran Ltd accept no responsibility for accuracy of data |
|
Back to Materials
|
|
|
Membership Crystran Ltd is proud to be ISO 9001 certified through LRQA and ISO
14001 certified through SGS. |
| |
|